Magnetron deposition of ceramic oxide-superconductor thin films

Assignee: Individual
•
Filing: 1987-07-29
•
Granted: 1989-06-27
•
Expires: 2007-07-29
📄 Original PDF 🌐 Google Patents 🔄 Sync Now

Abstract

Abstract A method for depositing and tailoring anisotropic properties of ceramic oxide superconductive films onto the outer surface of fibers, wires, rods, bars and onto the inner surface of tubes, as well as onto the surface of disc-shaped substrates, employs either tandem magnetron discharges alone or both an abnormal glow cold cathode electron gun together with tandem magnetron discharges. This deposition method provides uniform thin films having high growth rates, controllable stoichiometry and desired anisotropic microstructure. The magnetron cathodes are made from either mixtures or single elements of the metals. The oxygen component is achieved either from the cathode material itself or by reactive sputtering in an oxygen ambient or a post-deposition thermal or plasma oxidation. An external electron beam may also be used for in-situ annealing of the deposited films while placed under an external applied magnetic field to better align crystals in the films for the desired anisotropic superconducting properties. Thin metal or dielectric thin films are deposited as an interface layer and are placed both on the top of and under the metal oxide ceramic superconductive film material. Hermetic seal layers are deposited to protect the ceramic oxide superconductive films from being poisoned by foreign atoms.

Inventors

  • 👤 George J. Collins
  • 👤 John R. McNeil
  • 👤 Zeng-gi Yu

Bibliographic Details

Application Number —
Jurisdiction US
Data Source google_patents
Last Synchronized 2026-10-29 06:59
CPC Classifications
H; H10; H10N; H10N60/00; H10N60/01; H10N60/0268; H10N60/0801; C; C23; C23C; C23C14/00; C23C14/22; C23C14/34; C23C14/3435; C23C14/35; C23C14/354; C23C14/355; C23C14/56; C23C14/562; C30; C30B; C30B13/00; C30B29/00; C30B29/10; C30B29/16; C30B29/22; C30B29/225; H01; H01J; H01J37/00; H01J37/32; H01J37/32431; H01J37/32733; H01J37/32752; H01J37/32761; H01J37/3277; H01J37/34; H01J37/3411; H01J37/3414; H01J37/342; H01J37/3438; H10N60/0296; H10N60/0408; H10N60/0661; H10N60/0716; Y; Y10; Y10S; Y10S505/00; Y10S505/80; Y10S505/815; Y10S505/816

Claims Analysis

Total Claims: 66
Claim 1
Independent Claim 252 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the one or more sputtered ternary metal materials to form the film of metal oxide ceramic materials.
Claim 2
Independent Claim 252 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the one or more sputtered ternary metal materials to form the film of metal oxide ceramic materials.
Claim 3
Independent Claim 212 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising a ternary mixture of metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron such that the metal oxide ceramic materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate.
Claim 4
Independent Claim 212 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising a ternary mixture of metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron such that the metal oxide ceramic materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate.
Claim 5
Independent Claim 269 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, each having a cylindrical extraction grid coaxially positioned with respect to the substrate, each having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, each having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, each cylindrical cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas including oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons such that the elemental metal materials comprising the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; and subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials.
Claim 6
Independent Claim 269 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, each having a cylindrical extraction grid coaxially positioned with respect to the substrate, each having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, each having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, each cylindrical cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas including oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons such that the elemental metal materials comprising the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; and subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials.
Claim 7
Independent Claim 248 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials.
Claim 8
Independent Claim 248 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials.
Claim 9
Independent Claim 211 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron such that the metal oxide ceramic materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate.
Claim 10
Independent Claim 211 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron such that the metal oxide ceramic materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate.
Claim 11
Independent Claim 272 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons each having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, each having a cylindrical extraction grid coaxially positioned with respect to the substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, each having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, each cylindrical cathode comprising a single elemental metal material, and each of said plurality of tandem cylindrical magetrons having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas that includes oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons such that the elemental metal materials comprising the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; and subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials.
Claim 12
Independent Claim 272 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons each having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, each having a cylindrical extraction grid coaxially positioned with respect to the substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, each having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, each cylindrical cathode comprising a single elemental metal material, and each of said plurality of tandem cylindrical magetrons having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas that includes oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons such that the elemental metal materials comprising the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; and subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials.
Claim 13
Independent Claim 326 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical anode coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the one or more sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 14
Independent Claim 326 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical anode coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the one or more sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 15
Independent Claim 292 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical anode coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas that includes oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 16
Independent Claim 292 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical anode coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas that includes oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 17
Independent Claim 353 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, each having a cylindrical anode coaxially positioned with respect to the substrate, each having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, each of the cylindrical cathodes comprising a single elemental metal material, and each of the plurality of tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 18
Independent Claim 353 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, each having a cylindrical anode coaxially positioned with respect to the substrate, each having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, each of the cylindrical cathodes comprising a single elemental metal material, and each of the plurality of tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 19
Independent Claim 346 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 20
Independent Claim 346 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 21
Independent Claim 319 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode o diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas that comprises oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 22
Independent Claim 319 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode o diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas that comprises oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 23
Independent Claim 380 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, each having a cylindrical extraction grid coaxially positioned with respect to the substrate, each having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, each having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, each cylindrical cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more rare gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 24
Independent Claim 380 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, each having a cylindrical extraction grid coaxially positioned with respect to the substrate, each having a cylindrical anode of diameter greater than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, each having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, each cylindrical cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more rare gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 25
Independent Claim 346 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 26
Independent Claim 346 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 27
Independent Claim 319 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas that comprises oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 28
Independent Claim 319 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, having a cylindrical extraction grid coaxially positioned with respect to the substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, said cylindrical cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas that comprises oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the cylindrical cathode are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 29
Independent Claim 380 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, each having a cylindrical extraction grid coaxially positioned with respect to the substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, each having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, each cylindrical cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more rare gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 30
Independent Claim 380 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the outer surface of a substrate, the method comprising: introducing a substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the substrate, each having a cylindrical extraction grid coaxially positioned with respect to the substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the substrate, each having a cylindrical cathode of diameter greater than that of the cylindrical anode and coaxially positioned with respect to the substrate and the cylindrical anode, each cylindrical cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical cathode and coaxially positioned with respect to the substrate, the cylindrical extraction grid, the cylindrical cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more rare gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the outer surface of the substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 31
Independent Claim 275 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials.
Claim 32
Independent Claim 275 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials.
Claim 33
Independent Claim 237 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron such that the metal oxide ceramic materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the substrate.
Claim 34
Independent Claim 237 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron such that the metal oxide ceramic materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the substrate.
Claim 35
Independent Claim 297 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, each having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, each having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, each post cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas including oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons such that the elemental metal materials comprising the post cathodes are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; and subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the cylindrical substrate to form the film of metal oxide ceramic materials.
Claim 36
Independent Claim 297 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, each having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, each having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, each post cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas including oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons such that the elemental metal materials comprising the post cathodes are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; and subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the cylindrical substrate to form the film of metal oxide ceramic materials.
Claim 37
Independent Claim 266 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials.
Claim 38
Independent Claim 266 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials.
Claim 39
Independent Claim 229 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron such that the metal oxide ceramic materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate.
Claim 40
Independent Claim 229 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron such that the metal oxide ceramic materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate.
Claim 41
Independent Claim 290 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons each having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, each having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, each having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, each post cathode comprising a single elemental metal material, and each of said plurality of tandem cylindrical magetrons having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas that includes oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons such that the elemental metal materials comprising the post cathodes are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; and subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials.
Claim 42
Independent Claim 290 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons each having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, each having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, each having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, each post cathode comprising a single elemental metal material, and each of said plurality of tandem cylindrical magetrons having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas that includes oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons such that the elemental metal materials comprising the post cathodes are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; and subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the substrate to form the film of metal oxide ceramic materials.
Claim 43
Independent Claim 341 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 44
Independent Claim 341 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 45
Independent Claim 309 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the post cathode and coaxially positioned with respect to the cylindrical substrate, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas that includes oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 46
Independent Claim 309 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the post cathode and coaxially positioned with respect to the cylindrical substrate, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a sputter gas that includes oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 47
Independent Claim 373 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, each having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, each of the post cathodes comprising a single elemental metal material, and each of the plurality of tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the post cathodes are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the cylindrical substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the plurality of cylindrical magnetrons such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 48
Independent Claim 373 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, each having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, each of the post cathodes comprising a single elemental metal material, and each of the plurality of tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the post cathodes are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the cylindrical substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the plurality of cylindrical magnetrons such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 49
Independent Claim 373 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 50
Independent Claim 373 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 51
Independent Claim 346 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of said cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the coaxial substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas that comprises oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 52
Independent Claim 346 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of said cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the coaxial substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas that comprises oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 53
Independent Claim 407 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, each having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, each having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, each post cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more rare gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the cylindrical substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the plurality of cylindrical magnetrons such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 54
Independent Claim 407 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, each having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical substrate but greater than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, each having a post cathode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, each post cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more rare gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the cylindrical cathodes are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the cylindrical substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the plurality of cylindrical magnetrons such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 55
Independent Claim 364 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that or the cylindrical anode and coaxially positioned with respect tot he cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 56
Independent Claim 364 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that or the cylindrical anode and coaxially positioned with respect tot he cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the cylindrical magnetron such that the metal materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate and such that a cylindrical magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the sputtered metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 57
Independent Claim 337 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas that comprises oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 58
Independent Claim 337 words
A method for deposition a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a cylindrical magnetron having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, said post cathode comprising at least three metal oxide ceramic materials, and having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the cylindrical magnetron into a plasma region of the cylindrical magnetron to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas that comprises oxygen and one or more inert gases; applying operating voltages to the elements of the cylindrical magnetron and the disc-shaped cold cathode such that the metal oxide ceramic materials of the post cathode are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 59
Independent Claim 396 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, each having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, each having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, each post cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more rare gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the post cathodes are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the cylindrical substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 60
Independent Claim 396 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto the inner surface of a cylindrical substrate, the method comprising: introducing a cylindrical substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem cylindrical magnetrons, each having a longitudinal axis substantially coincident with a longitudinal axis of the cylindrical substrate, each having a cylindrical extraction grid of diameter smaller than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, each having a cylindrical anode of diameter smaller than that of the cylindrical extraction grid and coaxially positioned with respect to the cylindrical substrate, each having a post cathode of diameter smaller than that of the cylindrical anode and coaxially positioned with respect to the cylindrical substrate and the cylindrical anode, each post cathode comprising a single elemental metal material, and each of said tandem cylindrical magnetrons having a cylindrical solenoid of diameter greater than that of the cylindrical substrate and coaxially positioned with respect to the cylindrical substrate, the cylindrical extraction grid, the post cathode, and the cylindrical anode; injecting a beam of energetic electrons created by a disc-shaped cold cathode positioned proximate to one end of the plurality of tandem cylindrical magnetrons into a plasma region of the plurality of tandem cylindrical magnetrons to sustain a magnetron discharge; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more rare gases; applying operating voltages to the elements of the plurality of tandem cylindrical magnetrons and the disc-shaped cold cathode such that the elemental metal materials of the post cathodes are sputtered therefrom and deposited uniformly onto the inner surface of the cylindrical substrate; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the cylindrical substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film by causing impingement upon the deposited superconducting thin film by a disc-shaped beam of electrons produced by a ring-shaped cold cathode positioned proximate to one end of the cylindrical magnetron such that crystallites therein are aligned with respect to a desired direction of anisotropic properties in response to a magnetic field created by the cylindrical solenoid.
Claim 61
Independent Claim 276 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto a surface of a wide area planar substrate, the method comprising: introducing a planar substrate to be coated into a vacuum chamber apparatus that includes a planar magnetron having a normal axis substantially coincident with a normal axis of the planar substrate, having a planar extraction grid positioned parallel to the planar substrate, having a planar anode positioned parallel to the planar substrate, having a planar cathode positioned parallel to the planar substrate, said planar cathode comprising at least three metal materials, and having a magnetic field means positioned parallel to the planar substrate for directing a focused magnetic field onto a surface of the planar substrate to be coated; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the planar magnetron such that the metal materials of the planar cathode are sputtered therefrom and deposited uniformly onto the surface of the planar substrate to be coated and such that a planar magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the one or more sputtered ternary metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film such that crystallites therein are aligned with respect to a desired direction of anisotropic properties by causing impingement upon the deposited superconducting thin film by a line-shaped beam of electrons produced by a line-shaped cold cathode positioned parallel to the planar substrate.
Claim 62
Independent Claim 276 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto a surface of a wide area planar substrate, the method comprising: introducing a planar substrate to be coated into a vacuum chamber apparatus that includes a planar magnetron having a normal axis substantially coincident with a normal axis of the planar substrate, having a planar extraction grid positioned parallel to the planar substrate, having a planar anode positioned parallel to the planar substrate, having a planar cathode positioned parallel to the planar substrate, said planar cathode comprising at least three metal materials, and having a magnetic field means positioned parallel to the planar substrate for directing a focused magnetic field onto a surface of the planar substrate to be coated; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising an inert gas and a reactive gas mixture comprising at least oxygen; applying operating voltages to the elements of the planar magnetron such that the metal materials of the planar cathode are sputtered therefrom and deposited uniformly onto the surface of the planar substrate to be coated and such that a planar magnetron plasma dissociates the reactive gas mixture into oxygen atoms to enhance oxidation of the one or more sputtered ternary metal materials to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film such that crystallites therein are aligned with respect to a desired direction of anisotropic properties by causing impingement upon the deposited superconducting thin film by a line-shaped beam of electrons produced by a line-shaped cold cathode positioned parallel to the planar substrate.
Claim 63
Independent Claim 237 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto a surface of a wide area planar substrate, the method comprising: introducing a planar substrate to be coated into a vacuum chamber apparatus that includes a planar magnetron having a normal axis substantially coincident with a normal axis of the planar substrate, having a planar extraction grid positioned parallel to the planar substrate, having a planar anode positioned parallel to the planar substrate, having a planar cathode positioned parallel to the planar substrate, said planar cathode comprising at least three metal oxide materials, and having a magnetic field means positioned parallel to the planar substrate for directing a focused magnetic field onto a surface of the planar substrate to be coated; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more inert gases; applying operating voltages to the elements of the planar magnetron such that the metal oxide materials of the planar cathode are sputtered therefrom and deposited uniformly onto the surface of the planar substrate to be coated; and thermally annealing the deposited superconducting thin film such that crystallites therein are aligned with respect to a desired direction of anisotropic properties by causing impingement upon the deposited superconducting thin film by a line-shaped beam of electrons produced by a line-shaped cold cathode positioned parallel to the planar substrate.
Claim 64
Independent Claim 237 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto a surface of a wide area planar substrate, the method comprising: introducing a planar substrate to be coated into a vacuum chamber apparatus that includes a planar magnetron having a normal axis substantially coincident with a normal axis of the planar substrate, having a planar extraction grid positioned parallel to the planar substrate, having a planar anode positioned parallel to the planar substrate, having a planar cathode positioned parallel to the planar substrate, said planar cathode comprising at least three metal oxide materials, and having a magnetic field means positioned parallel to the planar substrate for directing a focused magnetic field onto a surface of the planar substrate to be coated; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more inert gases; applying operating voltages to the elements of the planar magnetron such that the metal oxide materials of the planar cathode are sputtered therefrom and deposited uniformly onto the surface of the planar substrate to be coated; and thermally annealing the deposited superconducting thin film such that crystallites therein are aligned with respect to a desired direction of anisotropic properties by causing impingement upon the deposited superconducting thin film by a line-shaped beam of electrons produced by a line-shaped cold cathode positioned parallel to the planar substrate.
Claim 65
Independent Claim 301 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto a surface of a wide area planar substrate, the method comprising: introducing a planar substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem planar magnetrons, each having a normal axis substantially coincident with a normal axis of the planar substrate, each having a planar extraction grid positioned parallel to the planar substrate, each having a planar anode positioned parallel to the planar substrate, each having a planar cathode positioned parallel to the planar substrate, each planar cathode comprising a single elemental metal material, and each of said tandem planar magnetrons having a magnetic field means for positioned parallel to the planar substrate for directing a focused magnetic field onto a surface of the planar substrate to be coated; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem planar magnetrons such that the elemental metal materials of the planar cathodes cathodes are sputtered therefrom and deposited uniformly onto the surface of the planar substrate to be coated; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the surface to be coated of the planar substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film such that crystallites therein are aligned with respect to a desired direction of anisotropic properties by causing impingement upon the deposited superconducting thin film by a line-shaped beam of electrons produced by a line-shaped cold cathode positioned parallel to the planar substrate.
Claim 66
Independent Claim 301 words
A method for depositing a superconducting thin film of metal oxide ceramic materials onto a surface of a wide area planar substrate, the method comprising: introducing a planar substrate to be coated into a vacuum chamber apparatus that includes a plurality of tandem planar magnetrons, each having a normal axis substantially coincident with a normal axis of the planar substrate, each having a planar extraction grid positioned parallel to the planar substrate, each having a planar anode positioned parallel to the planar substrate, each having a planar cathode positioned parallel to the planar substrate, each planar cathode comprising a single elemental metal material, and each of said tandem planar magnetrons having a magnetic field means for positioned parallel to the planar substrate for directing a focused magnetic field onto a surface of the planar substrate to be coated; establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere including a sputter gas comprising oxygen and one or more inert gases; applying operating voltages to the elements of the plurality of tandem planar magnetrons such that the elemental metal materials of the planar cathodes cathodes are sputtered therefrom and deposited uniformly onto the surface of the planar substrate to be coated; subsequently establishing a controlled gas atmosphere within the vacuum chamber apparatus, the controlled gas atmosphere comprising a rare gas-oxygen atmosphere to plasma oxidize the elemental metal materials deposited onto the surface to be coated of the planar substrate to form the film of metal oxide ceramic materials; and thermally annealing the deposited superconducting thin film such that crystallites therein are aligned with respect to a desired direction of anisotropic properties by causing impingement upon the deposited superconducting thin film by a line-shaped beam of electrons produced by a line-shaped cold cathode positioned parallel to the planar substrate.

References Cited (Backward Citations)

US4031424A Cited
US4530750A Cited
JPH0696599A Cited

USPTO Annuity & Maintenance Windows

Annuity Stage Window Opens Payment Deadline Surcharge Period Until Estimated Fee Status
3.5 Years (Year 4) 1992-06-26 1992-12-26 1993-06-27 $2000.00 Window Closed / Lapsed
7.5 Years (Year 8) 1996-06-26 1996-12-26 1997-06-27 $3760.00 Window Closed / Lapsed
11.5 Years (Year 12) 2000-06-26 2000-12-26 2001-06-27 $7700.00 Window Closed / Lapsed