← Back to Patent Explorer
US4282120A Expired / Lapsed US ⏱️ 0.0 years remaining

Sheet material for general coverings and method of making the same

Assignee: Sub Utilizzazione Brevetti Srl Soc
•
Filing: 1978-01-25
•
Granted: 1981-08-04
•
Expires: 1998-01-25
📄 Original PDF 🌐 Google Patents 🔄 Sync Now

Abstract

Abstract Method of producing a stratiform material, wherein 35-45 parts by weight of solvents for polyvinylacetate (PVA) homopolymer in the form of flakes or pearls are stirred with 10-15 parts of PVA and 2-5 parts by weight of oil, while separately mixing 25-30% by weight of wood powder having a granulometry in the range of 50-150 microns and mineral fillers in an amount of 10-20% by weight, then intermixing the liquid and powdery phases to obtain a homogeneous mixture which is passed through calendering rollers, the last pair of which produces an embossing on at least one of the two surfaces, the layer being reduced to a thickness in the range of 0.2-2.0 millimeters.

Inventors

  • 👤 Leandro Cisterni

Bibliographic Details

Application Number —
Jurisdiction US
Data Source google_patents
Last Synchronized 2026-11-04 16:56
CPC Classifications
C; C08; C08L; C08L97/00; C08L97/02; C08K; C08K3/00; C08K3/01; C08K3/013; C08K5/00; C08K5/01; C08L29/00; C08L29/02; C08L29/04; C08L31/00; C08L31/02; C08L31/04; Y; Y10; Y10T; Y10T428/00; Y10T428/25; Y10T428/253

Claims Analysis

Total Claims: 10
Claim 1
Independent Claim 110 words
A method of producing a stratiform material comprising stirring 35-45 parts by weight of solvents, polyvinylacetate homopolymer in the form of flakes or pearls with 10-15 parts of polyvinylacetate and 2-5 parts by weight of oil, separately mixing 25-30% by weight of wood powder having a granulometry in the range of 50-150 microns and mineral fillers in an amount of 10-20% by weight, then intermixing the liquid and powdery phases to obtain a homogeneous mixture which is passed through calendering rollers, the last pair of which produces an embossing on at least one of the two surfaces, the layer being reduced to a thickness in the range of 0.2-2.0 millimeters.
Claim 2
Independent Claim 110 words
A method of producing a stratiform material comprising stirring 35-45 parts by weight of solvents, polyvinylacetate homopolymer in the form of flakes or pearls with 10-15 parts of polyvinylacetate and 2-5 parts by weight of oil, separately mixing 25-30% by weight of wood powder having a granulometry in the range of 50-150 microns and mineral fillers in an amount of 10-20% by weight, then intermixing the liquid and powdery phases to obtain a homogeneous mixture which is passed through calendering rollers, the last pair of which produces an embossing on at least one of the two surfaces, the layer being reduced to a thickness in the range of 0.2-2.0 millimeters.
Claim 3
Dependent Claim 18 words
A method according to claim 1, wherein from the calendering outlet the product is introduced into an oven.
Claim 4
Dependent Claim 22 words
A method according to claim 1, wherein the products obtained are then stamped differentiating the wood veneerings by means of different colouring.
Claim 5
Dependent Claim 29 words
A method according to claim 1, wherein the percentages of the various ingredients are as follows: Solvents: 39.7% Oil: 4.0% Polyvinylacetate homopolymer: 13.2% Wood powder: 26.5% Mineral fillers: 16.6%
Claim 6
Dependent Claim 21 words
A method according to claim 4, wherein the solvents are a mixture of acetone and toluene of 26.5% and 13.2%, respectively.
Claim 7
Dependent Claim 28 words
A method according to claim 4, wherein the fillers are a mixture of inert materials in a percentage of 10.6%, and thixotropic agents in a percentage of 6.0%.
Claim 8
Dependent Claim 32 words
A process according to claim 1, wherein the percentages of the ingredients are as follows: Ash wood powder: 30.0% polyvinylacetate: 10.0% Acetone: 22.5% Toluene: 14.5% Hyperventilated magnesium silicate: 19.3% Silicone oil: 3.7%
Claim 9
Dependent Claim 18 words
A method of claim 6 wherein the inert material is calcium carbonate and the thioxtropic agents are Kaolinites.
Claim 10
Dependent Claim 10 words
A sheet material produced by the process of claim 1.

References Cited (Backward Citations)

GB242665A Cited
US2543101A Cited
US2790741A Cited
US3101241A Cited
US3114672A Cited
US3309444A Cited
US3287479A Cited
US3560324A Cited
US3718536A Cited
GB1362666A Cited
US3994845A Cited
US4112145A Cited

USPTO Annuity & Maintenance Windows

Annuity Stage Window Opens Payment Deadline Surcharge Period Until Estimated Fee Status
3.5 Years (Year 4) 1984-08-03 1985-02-02 1985-08-04 $2000.00 Window Closed / Lapsed
7.5 Years (Year 8) 1988-08-03 1989-02-02 1989-08-04 $3760.00 Window Closed / Lapsed
11.5 Years (Year 12) 1992-08-03 1993-02-02 1993-08-04 $7700.00 Window Closed / Lapsed

Assigned Categories & Tags

No categories assigned to this patent yet.

Assign Category Tag