Hybrid aligned liquid crystal display employing An anodized alignment layer and method for fabrication
Assignee: California Institute of Technology
•
Filing: 1996-03-07
•
Granted: 1999-03-09
•
Expires: 2016-03-07
Abstract
Abstract The present invention discloses nanomechanical fabrication methods of hybrid aligned nematic (HAN) cells of liquid crystals for creating analog spatial light modulators and smart pixel arrays on conventionally fabricated VLSI integrated circuits. The liquid crystal material is encapsulated between a top substrate and a bottom substrate. The locally averaged direction of the long axis of the molecules of liquid crystals of the HAN cells varies smoothly from homogeneous alignment on a top substrate to homeotropic alignment on a bottom substrate. The bottom substrate causes a homeotropic alignment of the liquid crystal because of its porous microstructure.
Inventors
- 👤 Axel Scherer
- 👤 Jean-Jacques P. Drolet
- 👤 Demetri Psaltis
Bibliographic Details
Application Number
—
Jurisdiction
US
Data Source
google_patents
Last Synchronized
2026-11-08 05:06
CPC Classifications
G; G02; G02F; G02F1/00; G02F1/01; G02F1/13; G02F1/133; G02F1/1333; G02F1/1337; G02F1/133742; G02F1/137; G02F1/13787; G02F1/139; G02F1/1393
Claims Analysis
Total Claims: 53
Claim 1
Independent Claim
119 words
A device having homeotropically aligned liquid crystals with respect to a surface of a substrate of said device, said device comprising: a film coating on said surface of said substrate; wherein said film is partially anodized in an acidic environment to form a porous layer on said film, said porous layer having elongated pores, each pore having a longitudinal axis, each of said longitudinal axes of said elongated pores being perpendicular to said surface of said substrate; and a liquid crystal material comprised of elongated molecules having a first portion overlying said porous layer, and a second portion residing within said elongated pores so that said elongated molecules are homeotropically aligned with respect to said surface of said substrate.
Claim 2
Independent Claim
119 words
A device having homeotropically aligned liquid crystals with respect to a surface of a substrate of said device, said device comprising: a film coating on said surface of said substrate; wherein said film is partially anodized in an acidic environment to form a porous layer on said film, said porous layer having elongated pores, each pore having a longitudinal axis, each of said longitudinal axes of said elongated pores being perpendicular to said surface of said substrate; and a liquid crystal material comprised of elongated molecules having a first portion overlying said porous layer, and a second portion residing within said elongated pores so that said elongated molecules are homeotropically aligned with respect to said surface of said substrate.
Claim 3
Dependent Claim
16 words
The invention as set forth in claim 1, wherein said liquid crystal is nematic liquid crystal.
Claim 4
Dependent Claim
16 words
The invention as set forth in claim 1, wherein said acidic environment is an acidic electrolyte.
Claim 5
Dependent Claim
20 words
The invention as set forth in claim 1, wherein said film is aluminum and said layer is porous aluminum oxide.
Claim 6
Dependent Claim
26 words
The invention as set forth in claim 1, wherein the diameter of the elongated pores is between the range of ten nanometers to three hundred nanometers.
Claim 7
Dependent Claim
18 words
The invention as set forth in claim 1, wherein the depth of the elongated pores is 1.5 micrometers.
Claim 8
Dependent Claim
26 words
The invention as set forth in claim 1, further comprising a top substrate overlying said film coating and said first portion of said liquid crystal material.
Claim 9
Dependent Claim
23 words
The invention as set forth in claim 7, wherein said elongated molecules of said first portion near said top substrate are homogeneously aligned.
Claim 10
Independent Claim
129 words
A method for creating homeotropic alignment, with respect to a surface of a substrate, of liquid crystals within a porous material, comprising the steps of: (a) coating said substrate with an aluminum film; (b) partially anodizing said film in an acidic environment to form a porous layer having elongated pores in a top region of said aluminum film, wherein each elongated pore has a longitudinal axis, and each of said longitudinal axes of said elongated pores are perpendicular to said surface of said substrate; and (c) depositing liquid crystal material comprised of elongated molecules onto said porous layer, whereby said liquid crystal flows into said elongated pores by capillary action so that said elongated molecules homeotropically align within said elongated pores, with respect to said surface of said substrate.
Claim 11
Independent Claim
129 words
A method for creating homeotropic alignment, with respect to a surface of a substrate, of liquid crystals within a porous material, comprising the steps of: (a) coating said substrate with an aluminum film; (b) partially anodizing said film in an acidic environment to form a porous layer having elongated pores in a top region of said aluminum film, wherein each elongated pore has a longitudinal axis, and each of said longitudinal axes of said elongated pores are perpendicular to said surface of said substrate; and (c) depositing liquid crystal material comprised of elongated molecules onto said porous layer, whereby said liquid crystal flows into said elongated pores by capillary action so that said elongated molecules homeotropically align within said elongated pores, with respect to said surface of said substrate.
Claim 12
Dependent Claim
16 words
The invention as set forth in claim 9, wherein said liquid crystal is nematic liquid crystal.
Claim 13
Dependent Claim
16 words
The invention as set forth in claim 9, wherein said acidic environment is an acidic electrolyte.
Claim 14
Dependent Claim
15 words
The invention as set forth in claim 9, wherein said layer is porous aluminum oxide.
Claim 15
Dependent Claim
26 words
The invention as set forth in claim 9, further comprising forming said elongated pores with a diameter in the range of 10 nm to 300 nm.
Claim 16
Dependent Claim
52 words
The invention as set forth in claim 9, further comprising the steps of placing a top substrate over said film coating and said first portion of said liquid crystal material and inducing, near said top substrate, homogeneous alignment of said elongated molecules of said first portion with respect to said top substrate.
Claim 17
Dependent Claim
164 words
A hybrid aligned nematic cell on an integrated circuit, comprising: a top substrate having an alignment film; a bottom substrate located on said integrated circuit; wherein said bottom substrate is anodized in an acidic environment to form a porous layer on said film, said porous layer having elongated pores, each pore having a longitudinal axis, each of said longitudinal axes of said elongated pores being perpendicular to said surface of said substrate; a liquid crystal material comprised of elongated molecules having a first portion near said top substrate and overlying said porous layer, and a second portion residing within said elongated pores so that said elongated molecules are homeotropically aligned with respect to said surface of said substrate; and wherein said elongated molecules of said first portion near said top substrate are homogeneously aligned with respect to said alignment film and wherein said homogeneously aligned elongated molecules near said top substrate vary smoothly in a splay-bend conformation to homeotropic alignment at said bottom substrate.
Claim 18
Dependent Claim
164 words
A hybrid aligned nematic cell on an integrated circuit, comprising: a top substrate having an alignment film; a bottom substrate located on said integrated circuit; wherein said bottom substrate is anodized in an acidic environment to form a porous layer on said film, said porous layer having elongated pores, each pore having a longitudinal axis, each of said longitudinal axes of said elongated pores being perpendicular to said surface of said substrate; a liquid crystal material comprised of elongated molecules having a first portion near said top substrate and overlying said porous layer, and a second portion residing within said elongated pores so that said elongated molecules are homeotropically aligned with respect to said surface of said substrate; and wherein said elongated molecules of said first portion near said top substrate are homogeneously aligned with respect to said alignment film and wherein said homogeneously aligned elongated molecules near said top substrate vary smoothly in a splay-bend conformation to homeotropic alignment at said bottom substrate.
Claim 19
Dependent Claim
30 words
The invention as set forth in claim 15, further comprising spacers affixed to said bottom substrate so that said top substrate is a spaced apart distance from said bottom substrate.
Claim 20
Dependent Claim
25 words
The invention as set forth in claim 15, wherein said hybrid aligned nematic cell is an analog spatial light modulator fabricated on said integrated circuit.
Claim 21
Dependent Claim
22 words
The invention as set forth in claim 15, wherein said top substrate is a cover glass plate coated with a transparent electrode.
Claim 22
Dependent Claim
17 words
The invention as set forth in claim 18, wherein said transparent electrode is covered with rubbed polyimide.
Claim 23
Dependent Claim
21 words
The invention as set forth in claim 15, wherein said layer formed on said bottom substrate is partially anodized aluminum oxide.
Claim 24
Dependent Claim
31 words
The invention as set forth in claim 20, wherein said partially anodized aluminum has a remaining portion of aluminum defining metal electrodes that optically reflect light incident on said metal electrodes.
Claim 25
Dependent Claim
31 words
The invention as set forth in claim 21, wherein said metal electrodes are also contacts for applying voltages across said hybrid aligned nematic cell, thereby defining pixels having local processing functions.
Claim 26
Dependent Claim
32 words
The invention as set forth in claim 21, wherein said metal electrodes simultaneously apply local electric fields across said hybrid aligned nematic cell and optically reflect light incident on said metal electrodes.
Claim 27
Independent Claim
150 words
A method for creating a hybrid aligned nematic cell on an integrated circuit, comprising the steps of: (a) anodizing a bottom substrate in an acidic environment to form a porous layer having elongated pores in a top region of said bottom substrate, wherein each elongated pore has a longitudinal axis, and each of said longitudinal axes of said elongated pores are perpendicular to said surface of said bottom substrate; (b) placing a top substrate over said bottom substrate, thereby forming a cavity; (c) depositing liquid crystal comprised of elongated molecules between said top substrate and said bottom substrate into said cavity and onto said porous layer, whereby said liquid crystal flows into said elongated pores by capillary action so that said elongated molecules homeotropically align within said elongated pores, with respect to said surface of said substrate; and (d) inducing homogeneous alignment of said liquid crystals near said top substrate.
Claim 28
Independent Claim
150 words
A method for creating a hybrid aligned nematic cell on an integrated circuit, comprising the steps of: (a) anodizing a bottom substrate in an acidic environment to form a porous layer having elongated pores in a top region of said bottom substrate, wherein each elongated pore has a longitudinal axis, and each of said longitudinal axes of said elongated pores are perpendicular to said surface of said bottom substrate; (b) placing a top substrate over said bottom substrate, thereby forming a cavity; (c) depositing liquid crystal comprised of elongated molecules between said top substrate and said bottom substrate into said cavity and onto said porous layer, whereby said liquid crystal flows into said elongated pores by capillary action so that said elongated molecules homeotropically align within said elongated pores, with respect to said surface of said substrate; and (d) inducing homogeneous alignment of said liquid crystals near said top substrate.
Claim 29
Dependent Claim
49 words
The invention as set forth in claim 24, further comprising, after the step of placing a top substrate over said bottom substrate, the step of affixing spacers to said bottom substrate so that said top substrate is a spaced apart distance from said bottom substrate, thereby defining a cavity.
Claim 30
Dependent Claim
20 words
The invention as set forth in claim 24, wherein said layer of said bottom substrate is partially anodized aluminum oxide.
Claim 31
Dependent Claim
31 words
The invention as set forth in claim 26, wherein said partially anodized aluminum has a remaining portion of aluminum defining metal electrodes that optically reflect light incident on said metal electrodes.
Claim 32
Dependent Claim
31 words
The invention as set forth in claim 27, wherein said metal electrodes are also contacts for applying voltages across said hybrid aligned nematic cell, thereby defining pixels having local processing functions.
Claim 33
Dependent Claim
35 words
The invention as set forth in claim 27, further comprising the steps of simultaneously applying and reflecting local electric fields across said hybrid aligned nematic cell and reflecting optically light incident on said metal electrodes.
Claim 34
Dependent Claim
42 words
The invention as set forth in claim 29, further comprising the step of exposing selectively said aluminum so that the entire surface of said integrated circuit is covered with a passivation layer, except for said metal electrodes assigned to driving said pixels.
Claim 35
Dependent Claim
66 words
The invention as set forth in claim 24, further comprising the step of selectively anodizing said metal electrodes driving respective pixels by immersing said bottom substrate in an acidic electrolyte bath and circulating an ionic current between said bottom substrate and an external metal electrode, whereby a layer of porous aluminum oxide is formed on a top side of each metal electrode associated with individual pixels.
Claim 36
Dependent Claim
33 words
The invention as set forth in claim 24, further comprising, after the step of anodizing said bottom substrate in an acidic environment, the step of heating said bottom substrate above a clearing point.
Claim 37
Dependent Claim
52 words
The invention as set forth in claim 32, further comprising, after the step of contacting said liquid crystal with said bottom substrate, the step of allowing said bottom substrate to slowly cool down and equilibrate, whereby said hybrid aligned nematic cell enters a nematic phase transition before said liquid crystals homeotropically align.
Claim 38
Independent Claim
149 words
A device having homeotropically aligned liquid crystals with respect to a surface of a substrate of said device, said device comprising: a film coating on said surface of said substrate; wherein said film is anodized in an acidic environment to form a porous layer on said film, said porous layer having elongated pores, each pore having a longitudinal axis, each of said longitudinal axes of said elongated pores being perpendicular to said surface of said substrate; a liquid crystal material comprised of elongated molecules having a first portion overlying said porous layer, and a second portion residing within said elongated pores so that said elongated molecules are homeotropically aligned with respect to said surface of said substrate; a top substrate overlying said film coating and said first portion of said liquid crystal material; and wherein said elongated molecules of said first portion near said top substrate are homogeneously aligned.
Claim 39
Independent Claim
149 words
A device having homeotropically aligned liquid crystals with respect to a surface of a substrate of said device, said device comprising: a film coating on said surface of said substrate; wherein said film is anodized in an acidic environment to form a porous layer on said film, said porous layer having elongated pores, each pore having a longitudinal axis, each of said longitudinal axes of said elongated pores being perpendicular to said surface of said substrate; a liquid crystal material comprised of elongated molecules having a first portion overlying said porous layer, and a second portion residing within said elongated pores so that said elongated molecules are homeotropically aligned with respect to said surface of said substrate; a top substrate overlying said film coating and said first portion of said liquid crystal material; and wherein said elongated molecules of said first portion near said top substrate are homogeneously aligned.
Claim 40
Independent Claim
168 words
A method for creating homeotropic alignment, with respect to a surface of a substrate, of liquid crystals within a porous material, comprising the steps of: (a) coating said substrate with an aluminum film; (b) anodizing said substrate in an acidic environment to form a porous layer having elongated pores in a top region of said aluminum film, wherein each elongated pore has a longitudinal axis, and each of said longitudinal axes of said elongated pores are perpendicular to said surface of said substrate; (c) depositing liquid crystal material comprised of elongated molecules onto said porous layer, whereby said liquid crystal flows into said elongated pores by capillary action so that said elongated molecules homeotropically align within said elongated pores, with respect to said surface of said substrate; (d) placing a top substrate over said film coating and said first portion of said liquid crystal material; and (e) inducing near said top substrate, homogeneous alignment of said elongated molecules of said first portion with respect to said top substrate.
Claim 41
Independent Claim
168 words
A method for creating homeotropic alignment, with respect to a surface of a substrate, of liquid crystals within a porous material, comprising the steps of: (a) coating said substrate with an aluminum film; (b) anodizing said substrate in an acidic environment to form a porous layer having elongated pores in a top region of said aluminum film, wherein each elongated pore has a longitudinal axis, and each of said longitudinal axes of said elongated pores are perpendicular to said surface of said substrate; (c) depositing liquid crystal material comprised of elongated molecules onto said porous layer, whereby said liquid crystal flows into said elongated pores by capillary action so that said elongated molecules homeotropically align within said elongated pores, with respect to said surface of said substrate; (d) placing a top substrate over said film coating and said first portion of said liquid crystal material; and (e) inducing near said top substrate, homogeneous alignment of said elongated molecules of said first portion with respect to said top substrate.
Claim 42
Dependent Claim
63 words
A liquid crystal display comprising: a) a film located on a surface of a bottom substrate; b) the film having pores formed by an anodic process within; c) a liquid crystal material covering the pores; d) a top substrate covering the liquid crystal material; and e) the liquid crystal material being homeotropically aligned within the pores and homogeneously aligned near the top substrate.
Claim 43
Dependent Claim
63 words
A liquid crystal display comprising: a) a film located on a surface of a bottom substrate; b) the film having pores formed by an anodic process within; c) a liquid crystal material covering the pores; d) a top substrate covering the liquid crystal material; and e) the liquid crystal material being homeotropically aligned within the pores and homogeneously aligned near the top substrate.
Claim 44
Dependent Claim
14 words
The liquid crystal display of claim 36 wherein the film comprises a conductive material.
Claim 45
Dependent Claim
14 words
The liquid crystal display of claim 36 wherein the film comprises a reflective material.
Claim 46
Dependent Claim
12 words
The liquid crystal display of claim 36 wherein the film comprises aluminum.
Claim 47
Dependent Claim
18 words
The liquid crystal display of claim 39 wherein the aluminum film is partially anodized to form aluminum oxide.
Claim 48
Dependent Claim
21 words
The liquid crystal display of claim 40 wherein a portion of the aluminum film is unanodized so that it reflects light.
Claim 49
Dependent Claim
21 words
The liquid crystal display of claim 40 wherein a portion of the aluminum film is unanodized so that it conducts electricity.
Claim 50
Dependent Claim
32 words
The liquid crystal display of claim 42, wherein the aluminum forms electrodes, and wherein the application of voltage to the electrodes provides an electric field across the liquid crystal to define pixels.
Claim 51
Dependent Claim
31 words
The liquid crystal display of claim 36 wherein the homogeneously aligned liquid crystal material near the top substrate varies smoothly in a splay-bend conformation to homeotropic alignment near the bottom substrate.
Claim 52
Dependent Claim
14 words
The liquid crystal display of claim 36 wherein the bottom substrate is a semiconductor.
Claim 53
Dependent Claim
20 words
The liquid crystal display of claim 36 wherein the top substrate is a cover glass plate coated with transparent electrode.
References Cited (Backward Citations)
USPTO Annuity & Maintenance Windows
| Annuity Stage | Window Opens | Payment Deadline | Surcharge Period Until | Estimated Fee | Status |
|---|---|---|---|---|---|
| 3.5 Years (Year 4) | 2002-03-08 | 2002-09-07 | 2003-03-09 | $2000.00 | Window Closed / Lapsed |
| 7.5 Years (Year 8) | 2006-03-08 | 2006-09-07 | 2007-03-09 | $3760.00 | Window Closed / Lapsed |
| 11.5 Years (Year 12) | 2010-03-08 | 2010-09-07 | 2011-03-09 | $7700.00 | Window Closed / Lapsed |