← Back to Patent Explorer
US4061709A Expired / Lapsed US ⏱️ 0.0 years remaining

Manufacturing textured gloves of silicone rubber

Assignee: Dow Silicones Corp
•
Filing: 1975-06-25
•
Granted: 1977-12-06
•
Expires: 1995-06-25
📄 Original PDF 🌐 Google Patents 🔄 Sync Now

Abstract

Abstract There is described a method of manufacturing silicone rubber gloves with a non-blocking surface by repeatedly dipping a form in a solvent dispersion of uncured silicone rubber to build up a plurality of layers and then forming a layer of liquid droplets on the surface of the solvent-containing uncured rubber, thereby forming a textured surface as the solvent evaporates.

Inventors

  • 👤 Carl W. Miller
  • 👤 Lester C. Vandenberg
  • 👤 Wayne H. Statt

Bibliographic Details

Application Number —
Jurisdiction US
Data Source google_patents
Last Synchronized 2026-10-24 23:35
CPC Classifications
B; B29; B29C; B29C41/00; B29C41/02; B29C41/14; B29C37/00; B29C37/0067; B29D; B29D99/00; B29D99/0064; B29D99/0067; B29K; B29K2021/00; B29L; B29L2031/00; B29L2031/48; B29L2031/4842; B29L2031/4864

Claims Analysis

Total Claims: 5
Claim 1
Independent Claim 117 words
In a method of manufacturing textured gloves by repeatedly dipping a glove form into a solvent dispersion of uncured silicone rubber to build up a plurality of layers thereon followed by drying and curing the silicone rubber layers to form a glove, the additional step , prior to curing the layers, of exposing the uncured solvent-containing surface of the last layer of silicone rubber to a wet atmosphere as the solvent evaporates until a fine non-coalescing layer of fluid particles has been deposited over the surface of the last layer, the atmosphere being chosen so that the fluid particles have the same or greater heat of vaporization than said solvent whereby a texturized surface effect is produced.
Claim 2
Dependent Claim 117 words
In a method of manufacturing textured gloves by repeatedly dipping a glove form into a solvent dispersion of uncured silicone rubber to build up a plurality of layers thereon followed by drying and curing the silicone rubber layers to form a glove, the additional step , prior to curing the layers, of exposing the uncured solvent-containing surface of the last layer of silicone rubber to a wet atmosphere as the solvent evaporates until a fine non-coalescing layer of fluid particles has been deposited over the surface of the last layer, the atmosphere being chosen so that the fluid particles have the same or greater heat of vaporization than said solvent whereby a texturized surface effect is produced.
Claim 3
Dependent Claim 45 words
The method as defined in claim 1 wherein immediately prior to forming said layer of fluid particles the last layer of uncured rubber on the glove form is dried to evaporate the solvent, and is then immersed in the solvent for said uncured silicone rubber.
Claim 4
Dependent Claim 45 words
The method as defined in claim 2 wherein said layer of fluid particles is formed by exposing the surface of the uncured solvent-containing last layer of silicone rubber to a steam saturated atmosphere at a temperature less than 120° F. for at least 30 seconds.
Claim 5
Dependent Claim 45 words
The method as defined in claim 1 wherein said layer of fluid particles is formed by exposing the surface of the uncured solvent-containing last layer of silicone rubber to a steam saturated atmosphere at a temperature less than 120° F. for at least 30 seconds.

References Cited (Backward Citations)

US2064143A Cited
US2525272A Cited
US3255492A Cited
US3883899A Cited
US3872515A Cited

USPTO Annuity & Maintenance Windows

Annuity Stage Window Opens Payment Deadline Surcharge Period Until Estimated Fee Status
3.5 Years (Year 4) 1980-12-05 1981-06-06 1981-12-06 $2000.00 Window Closed / Lapsed
7.5 Years (Year 8) 1984-12-05 1985-06-06 1985-12-06 $3760.00 Window Closed / Lapsed
11.5 Years (Year 12) 1988-12-05 1989-06-06 1989-12-06 $7700.00 Window Closed / Lapsed